Resumo: | ABSTRACT: T91 ferritic-martensitic steel was exposed to Li, Na and K molten carbonates at 650??C under dynamic conditions up to 1000 h. After testing, three descaling methods, two from the ISO8407 and one from the ISO17245 stan-dards were applied to remove the corrosion products and determine the corrosion rates. The two ISO8407 methods were more appropriate although the procedure required several steps to fully remove the corrosion products. The ISO17245 method led to a higher mass loss affecting probably the base material. Oxides identi-fication was performed by XRD following step by step layers removal. Li-, Na-, K-containing oxides and chro-mates/chromites were detected. |
id |
RCAP_548b5fffb070d929e543f4a162078e59 |
---|---|
oai_identifier_str |
oai:repositorio.lneg.pt:10400.9/4013 |
network_acronym_str |
RCAP |
network_name_str |
Repositório Científico de Acesso Aberto de Portugal (Repositórios Cientìficos) |
repository_id_str |
7160 |
spelling |
Comparison of descaling methods to study the corrosion kinetics of ferritic steels after dynamic exposure to molten carbonatesMaterialsMolten carbonatesSteelHigh-temperature corrosionX-ray diffractionABSTRACT: T91 ferritic-martensitic steel was exposed to Li, Na and K molten carbonates at 650??C under dynamic conditions up to 1000 h. After testing, three descaling methods, two from the ISO8407 and one from the ISO17245 stan-dards were applied to remove the corrosion products and determine the corrosion rates. The two ISO8407 methods were more appropriate although the procedure required several steps to fully remove the corrosion products. The ISO17245 method led to a higher mass loss affecting probably the base material. Oxides identi-fication was performed by XRD following step by step layers removal. Li-, Na-, K-containing oxides and chro-mates/chromites were detected.ElsevierRepositório do LNEGAudigié, PaulineRodríguez Catela, SergioAgüero, AlinaPedrosa, FátimaPaiva Luís, TeresaCunha Diamantino, Teresa2023-02-10T15:31:16Z2022-122022-12-01T00:00:00Zinfo:eu-repo/semantics/publishedVersioninfo:eu-repo/semantics/articleapplication/pdfhttp://hdl.handle.net/10400.9/4013engAudigié, P... [et.al.] - Comparison of descaling methods to study the corrosion kinetics of ferritic steels after dynamic exposure to molten carbonates. In: Corrosion Science, 2022, vol. 209, article nº 1107860010-938X10.1016/j.corsci.2022.1107861879-0496info:eu-repo/semantics/openAccessreponame:Repositório Científico de Acesso Aberto de Portugal (Repositórios Cientìficos)instname:Agência para a Sociedade do Conhecimento (UMIC) - FCT - Sociedade da Informaçãoinstacron:RCAAP2023-02-12T05:16:26Zoai:repositorio.lneg.pt:10400.9/4013Portal AgregadorONGhttps://www.rcaap.pt/oai/openaireopendoar:71602024-03-19T16:46:30.317631Repositório Científico de Acesso Aberto de Portugal (Repositórios Cientìficos) - Agência para a Sociedade do Conhecimento (UMIC) - FCT - Sociedade da Informaçãofalse |
dc.title.none.fl_str_mv |
Comparison of descaling methods to study the corrosion kinetics of ferritic steels after dynamic exposure to molten carbonates |
title |
Comparison of descaling methods to study the corrosion kinetics of ferritic steels after dynamic exposure to molten carbonates |
spellingShingle |
Comparison of descaling methods to study the corrosion kinetics of ferritic steels after dynamic exposure to molten carbonates Audigié, Pauline Materials Molten carbonates Steel High-temperature corrosion X-ray diffraction |
title_short |
Comparison of descaling methods to study the corrosion kinetics of ferritic steels after dynamic exposure to molten carbonates |
title_full |
Comparison of descaling methods to study the corrosion kinetics of ferritic steels after dynamic exposure to molten carbonates |
title_fullStr |
Comparison of descaling methods to study the corrosion kinetics of ferritic steels after dynamic exposure to molten carbonates |
title_full_unstemmed |
Comparison of descaling methods to study the corrosion kinetics of ferritic steels after dynamic exposure to molten carbonates |
title_sort |
Comparison of descaling methods to study the corrosion kinetics of ferritic steels after dynamic exposure to molten carbonates |
author |
Audigié, Pauline |
author_facet |
Audigié, Pauline Rodríguez Catela, Sergio Agüero, Alina Pedrosa, Fátima Paiva Luís, Teresa Cunha Diamantino, Teresa |
author_role |
author |
author2 |
Rodríguez Catela, Sergio Agüero, Alina Pedrosa, Fátima Paiva Luís, Teresa Cunha Diamantino, Teresa |
author2_role |
author author author author author |
dc.contributor.none.fl_str_mv |
Repositório do LNEG |
dc.contributor.author.fl_str_mv |
Audigié, Pauline Rodríguez Catela, Sergio Agüero, Alina Pedrosa, Fátima Paiva Luís, Teresa Cunha Diamantino, Teresa |
dc.subject.por.fl_str_mv |
Materials Molten carbonates Steel High-temperature corrosion X-ray diffraction |
topic |
Materials Molten carbonates Steel High-temperature corrosion X-ray diffraction |
description |
ABSTRACT: T91 ferritic-martensitic steel was exposed to Li, Na and K molten carbonates at 650??C under dynamic conditions up to 1000 h. After testing, three descaling methods, two from the ISO8407 and one from the ISO17245 stan-dards were applied to remove the corrosion products and determine the corrosion rates. The two ISO8407 methods were more appropriate although the procedure required several steps to fully remove the corrosion products. The ISO17245 method led to a higher mass loss affecting probably the base material. Oxides identi-fication was performed by XRD following step by step layers removal. Li-, Na-, K-containing oxides and chro-mates/chromites were detected. |
publishDate |
2022 |
dc.date.none.fl_str_mv |
2022-12 2022-12-01T00:00:00Z 2023-02-10T15:31:16Z |
dc.type.status.fl_str_mv |
info:eu-repo/semantics/publishedVersion |
dc.type.driver.fl_str_mv |
info:eu-repo/semantics/article |
format |
article |
status_str |
publishedVersion |
dc.identifier.uri.fl_str_mv |
http://hdl.handle.net/10400.9/4013 |
url |
http://hdl.handle.net/10400.9/4013 |
dc.language.iso.fl_str_mv |
eng |
language |
eng |
dc.relation.none.fl_str_mv |
Audigié, P... [et.al.] - Comparison of descaling methods to study the corrosion kinetics of ferritic steels after dynamic exposure to molten carbonates. In: Corrosion Science, 2022, vol. 209, article nº 110786 0010-938X 10.1016/j.corsci.2022.110786 1879-0496 |
dc.rights.driver.fl_str_mv |
info:eu-repo/semantics/openAccess |
eu_rights_str_mv |
openAccess |
dc.format.none.fl_str_mv |
application/pdf |
dc.publisher.none.fl_str_mv |
Elsevier |
publisher.none.fl_str_mv |
Elsevier |
dc.source.none.fl_str_mv |
reponame:Repositório Científico de Acesso Aberto de Portugal (Repositórios Cientìficos) instname:Agência para a Sociedade do Conhecimento (UMIC) - FCT - Sociedade da Informação instacron:RCAAP |
instname_str |
Agência para a Sociedade do Conhecimento (UMIC) - FCT - Sociedade da Informação |
instacron_str |
RCAAP |
institution |
RCAAP |
reponame_str |
Repositório Científico de Acesso Aberto de Portugal (Repositórios Cientìficos) |
collection |
Repositório Científico de Acesso Aberto de Portugal (Repositórios Cientìficos) |
repository.name.fl_str_mv |
Repositório Científico de Acesso Aberto de Portugal (Repositórios Cientìficos) - Agência para a Sociedade do Conhecimento (UMIC) - FCT - Sociedade da Informação |
repository.mail.fl_str_mv |
|
_version_ |
1799130936469618688 |