Synthesis and magnetic properties of the SiO2 BaFe12O19 glass ceramic composites
Autor(a) principal: | |
---|---|
Data de Publicação: | 2006 |
Outros Autores: | , , , |
Tipo de documento: | Artigo |
Idioma: | eng |
Título da fonte: | Repositório Institucional da UFRN |
Texto Completo: | https://repositorio.ufrn.br/jspui/handle/123456789/29194 |
Resumo: | Samples of the magnetic glass–ceramics SiO2–BaFe12O19 were obtained from mixtures of Fe2O3–BaSO4–SiO2–Na2CO3–CaCO3 following a two-step route. The samples were characterized using XRD analysis and scanning electron microscopy, and their room temperature magnetization hysteresis loops were measured. It was found that the magnetic phase was completely developed in the precursor BaFe12O19 material when it was calcinated above 1000 °C. The size of the particles of the BaFe12O19 phase depends on the thermal treatment conditions and on the SiO2 concentration. The magnetic data showed that the high value of the coercive magnetic field is preserved despite the fact that both the remanent and the saturation magnetizations diminish substantially |
id |
UFRN_fea01b6afe93cab38bf1b69fbc587bf2 |
---|---|
oai_identifier_str |
oai:https://repositorio.ufrn.br:123456789/29194 |
network_acronym_str |
UFRN |
network_name_str |
Repositório Institucional da UFRN |
repository_id_str |
|
spelling |
Araújo, José Humberto deCabral, F. A. O.Ginani, Marconi FloripeSoares, João MariaMachado, Fernando. L. A.2020-06-09T17:57:00Z2020-06-09T17:57:00Z2006-09-15ARAUJO, J; CABRAL, F ; GINANI, M ; SOARES, J ; MACHADO, F.. Synthesis and magnetic properties of the SiO2 BaFe12O19 glass ceramic composites. Journal of Non-Crystalline Solids, v. 352, p. 3518-3521, 2006. Disponível em: https://www.sciencedirect.com/science/article/abs/pii/S0022309306007800?via%3Dihub#!. Acesso em: 01 jun 2020. https://doi.org/10.1016/j.jnoncrysol.2006.03.107 .0022-3093https://repositorio.ufrn.br/jspui/handle/123456789/2919410.1016/j.jnoncrysol.2006.03.107ElsevierAttribution 3.0 Brazilhttp://creativecommons.org/licenses/by/3.0/br/info:eu-repo/semantics/openAccessGlass formationMagnetic propertiesSoda-lime–silicaSinteringSynthesis and magnetic properties of the SiO2 BaFe12O19 glass ceramic compositesinfo:eu-repo/semantics/publishedVersioninfo:eu-repo/semantics/articleSamples of the magnetic glass–ceramics SiO2–BaFe12O19 were obtained from mixtures of Fe2O3–BaSO4–SiO2–Na2CO3–CaCO3 following a two-step route. The samples were characterized using XRD analysis and scanning electron microscopy, and their room temperature magnetization hysteresis loops were measured. It was found that the magnetic phase was completely developed in the precursor BaFe12O19 material when it was calcinated above 1000 °C. The size of the particles of the BaFe12O19 phase depends on the thermal treatment conditions and on the SiO2 concentration. The magnetic data showed that the high value of the coercive magnetic field is preserved despite the fact that both the remanent and the saturation magnetizations diminish substantiallyengreponame:Repositório Institucional da UFRNinstname:Universidade Federal do Rio Grande do Norte (UFRN)instacron:UFRNORIGINALSynthesisAndMagneticProperties_Araujo_2006.pdfSynthesisAndMagneticProperties_Araujo_2006.pdfapplication/pdf713117https://repositorio.ufrn.br/bitstream/123456789/29194/4/SynthesisAndMagneticProperties_Araujo_2006.pdf2fe1f1be5c9ae8d68d7d45b39bd4f04bMD54CC-LICENSElicense_rdflicense_rdfapplication/rdf+xml; charset=utf-8914https://repositorio.ufrn.br/bitstream/123456789/29194/5/license_rdf4d2950bda3d176f570a9f8b328dfbbefMD55LICENSElicense.txtlicense.txttext/plain; charset=utf-81484https://repositorio.ufrn.br/bitstream/123456789/29194/6/license.txte9597aa2854d128fd968be5edc8a28d9MD56TEXTSynthesisAndMagneticProperties_Araujo_2006.pdf.txtSynthesisAndMagneticProperties_Araujo_2006.pdf.txtExtracted texttext/plain10811https://repositorio.ufrn.br/bitstream/123456789/29194/7/SynthesisAndMagneticProperties_Araujo_2006.pdf.txt0432fcbf0d695ba51d0847529cba127eMD57THUMBNAILSynthesisAndMagneticProperties_Araujo_2006.pdf.jpgSynthesisAndMagneticProperties_Araujo_2006.pdf.jpgGenerated Thumbnailimage/jpeg1727https://repositorio.ufrn.br/bitstream/123456789/29194/8/SynthesisAndMagneticProperties_Araujo_2006.pdf.jpg190fcb50a6dca2977d0d80ab650bd140MD58123456789/291942020-06-14 04:38:02.445oai:https://repositorio.ufrn.br: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Repositório de PublicaçõesPUBhttp://repositorio.ufrn.br/oai/opendoar:2020-06-14T07:38:02Repositório Institucional da UFRN - Universidade Federal do Rio Grande do Norte (UFRN)false |
dc.title.pt_BR.fl_str_mv |
Synthesis and magnetic properties of the SiO2 BaFe12O19 glass ceramic composites |
title |
Synthesis and magnetic properties of the SiO2 BaFe12O19 glass ceramic composites |
spellingShingle |
Synthesis and magnetic properties of the SiO2 BaFe12O19 glass ceramic composites Araújo, José Humberto de Glass formation Magnetic properties Soda-lime–silica Sintering |
title_short |
Synthesis and magnetic properties of the SiO2 BaFe12O19 glass ceramic composites |
title_full |
Synthesis and magnetic properties of the SiO2 BaFe12O19 glass ceramic composites |
title_fullStr |
Synthesis and magnetic properties of the SiO2 BaFe12O19 glass ceramic composites |
title_full_unstemmed |
Synthesis and magnetic properties of the SiO2 BaFe12O19 glass ceramic composites |
title_sort |
Synthesis and magnetic properties of the SiO2 BaFe12O19 glass ceramic composites |
author |
Araújo, José Humberto de |
author_facet |
Araújo, José Humberto de Cabral, F. A. O. Ginani, Marconi Floripe Soares, João Maria Machado, Fernando. L. A. |
author_role |
author |
author2 |
Cabral, F. A. O. Ginani, Marconi Floripe Soares, João Maria Machado, Fernando. L. A. |
author2_role |
author author author author |
dc.contributor.author.fl_str_mv |
Araújo, José Humberto de Cabral, F. A. O. Ginani, Marconi Floripe Soares, João Maria Machado, Fernando. L. A. |
dc.subject.por.fl_str_mv |
Glass formation Magnetic properties Soda-lime–silica Sintering |
topic |
Glass formation Magnetic properties Soda-lime–silica Sintering |
description |
Samples of the magnetic glass–ceramics SiO2–BaFe12O19 were obtained from mixtures of Fe2O3–BaSO4–SiO2–Na2CO3–CaCO3 following a two-step route. The samples were characterized using XRD analysis and scanning electron microscopy, and their room temperature magnetization hysteresis loops were measured. It was found that the magnetic phase was completely developed in the precursor BaFe12O19 material when it was calcinated above 1000 °C. The size of the particles of the BaFe12O19 phase depends on the thermal treatment conditions and on the SiO2 concentration. The magnetic data showed that the high value of the coercive magnetic field is preserved despite the fact that both the remanent and the saturation magnetizations diminish substantially |
publishDate |
2006 |
dc.date.issued.fl_str_mv |
2006-09-15 |
dc.date.accessioned.fl_str_mv |
2020-06-09T17:57:00Z |
dc.date.available.fl_str_mv |
2020-06-09T17:57:00Z |
dc.type.status.fl_str_mv |
info:eu-repo/semantics/publishedVersion |
dc.type.driver.fl_str_mv |
info:eu-repo/semantics/article |
format |
article |
status_str |
publishedVersion |
dc.identifier.citation.fl_str_mv |
ARAUJO, J; CABRAL, F ; GINANI, M ; SOARES, J ; MACHADO, F.. Synthesis and magnetic properties of the SiO2 BaFe12O19 glass ceramic composites. Journal of Non-Crystalline Solids, v. 352, p. 3518-3521, 2006. Disponível em: https://www.sciencedirect.com/science/article/abs/pii/S0022309306007800?via%3Dihub#!. Acesso em: 01 jun 2020. https://doi.org/10.1016/j.jnoncrysol.2006.03.107 . |
dc.identifier.uri.fl_str_mv |
https://repositorio.ufrn.br/jspui/handle/123456789/29194 |
dc.identifier.issn.none.fl_str_mv |
0022-3093 |
dc.identifier.doi.none.fl_str_mv |
10.1016/j.jnoncrysol.2006.03.107 |
identifier_str_mv |
ARAUJO, J; CABRAL, F ; GINANI, M ; SOARES, J ; MACHADO, F.. Synthesis and magnetic properties of the SiO2 BaFe12O19 glass ceramic composites. Journal of Non-Crystalline Solids, v. 352, p. 3518-3521, 2006. Disponível em: https://www.sciencedirect.com/science/article/abs/pii/S0022309306007800?via%3Dihub#!. Acesso em: 01 jun 2020. https://doi.org/10.1016/j.jnoncrysol.2006.03.107 . 0022-3093 10.1016/j.jnoncrysol.2006.03.107 |
url |
https://repositorio.ufrn.br/jspui/handle/123456789/29194 |
dc.language.iso.fl_str_mv |
eng |
language |
eng |
dc.rights.driver.fl_str_mv |
Attribution 3.0 Brazil http://creativecommons.org/licenses/by/3.0/br/ info:eu-repo/semantics/openAccess |
rights_invalid_str_mv |
Attribution 3.0 Brazil http://creativecommons.org/licenses/by/3.0/br/ |
eu_rights_str_mv |
openAccess |
dc.publisher.none.fl_str_mv |
Elsevier |
publisher.none.fl_str_mv |
Elsevier |
dc.source.none.fl_str_mv |
reponame:Repositório Institucional da UFRN instname:Universidade Federal do Rio Grande do Norte (UFRN) instacron:UFRN |
instname_str |
Universidade Federal do Rio Grande do Norte (UFRN) |
instacron_str |
UFRN |
institution |
UFRN |
reponame_str |
Repositório Institucional da UFRN |
collection |
Repositório Institucional da UFRN |
bitstream.url.fl_str_mv |
https://repositorio.ufrn.br/bitstream/123456789/29194/4/SynthesisAndMagneticProperties_Araujo_2006.pdf https://repositorio.ufrn.br/bitstream/123456789/29194/5/license_rdf https://repositorio.ufrn.br/bitstream/123456789/29194/6/license.txt https://repositorio.ufrn.br/bitstream/123456789/29194/7/SynthesisAndMagneticProperties_Araujo_2006.pdf.txt https://repositorio.ufrn.br/bitstream/123456789/29194/8/SynthesisAndMagneticProperties_Araujo_2006.pdf.jpg |
bitstream.checksum.fl_str_mv |
2fe1f1be5c9ae8d68d7d45b39bd4f04b 4d2950bda3d176f570a9f8b328dfbbef e9597aa2854d128fd968be5edc8a28d9 0432fcbf0d695ba51d0847529cba127e 190fcb50a6dca2977d0d80ab650bd140 |
bitstream.checksumAlgorithm.fl_str_mv |
MD5 MD5 MD5 MD5 MD5 |
repository.name.fl_str_mv |
Repositório Institucional da UFRN - Universidade Federal do Rio Grande do Norte (UFRN) |
repository.mail.fl_str_mv |
|
_version_ |
1814833074821660672 |