Powder diffraction of components subject to corrosion in fuse cutouts with ceramiclnsulation
Autor(a) principal: | |
---|---|
Data de Publicação: | 2008 |
Outros Autores: | , |
Tipo de documento: | Artigo de conferência |
Idioma: | eng |
Título da fonte: | Repositório Institucional da UNESP |
Texto Completo: | http://hdl.handle.net/11449/225385 |
Resumo: | Aiming identification of the components most affected by corrosion under saline environment conditions, we have carried out X-ray diffraction measurements in ceramic and bond materials, all in the powder form. The ceramic is analyzed before and after thermal annealing at 1000°C, showing the same DRX peaks, although better defined after annealing. Identification suggests the presence of Al6Si2O13 (Mullite) and SiO 2 (Quartz). Analysis of the junction (bond) material shows similar peaks, but a metallic preponderance is observed. Thermal annealing of the junction is done at much lower temperature, because it melts in the range 135°C-170°C, when a whitish smoke begins to show up along with strong sulfur odor. |
id |
UNSP_541bec336cc2b3d1aec52a854aaaa0c6 |
---|---|
oai_identifier_str |
oai:repositorio.unesp.br:11449/225385 |
network_acronym_str |
UNSP |
network_name_str |
Repositório Institucional da UNESP |
repository_id_str |
2946 |
spelling |
Powder diffraction of components subject to corrosion in fuse cutouts with ceramiclnsulationCeramicCorrosionFuse cutoutsMulliteX-ray diffractionAiming identification of the components most affected by corrosion under saline environment conditions, we have carried out X-ray diffraction measurements in ceramic and bond materials, all in the powder form. The ceramic is analyzed before and after thermal annealing at 1000°C, showing the same DRX peaks, although better defined after annealing. Identification suggests the presence of Al6Si2O13 (Mullite) and SiO 2 (Quartz). Analysis of the junction (bond) material shows similar peaks, but a metallic preponderance is observed. Thermal annealing of the junction is done at much lower temperature, because it melts in the range 135°C-170°C, when a whitish smoke begins to show up along with strong sulfur odor.Depto. Física - FC - UNESP POSMAT, Bauru - SPDepto. Física - FC - UNESP, Bauru - SPDepto. Química - FC - UNESP, Bauru - SPDepto. Física - FC - UNESP POSMAT, Bauru - SPDepto. Física - FC - UNESP, Bauru - SPDepto. Química - FC - UNESP, Bauru - SPUniversidade Estadual Paulista (UNESP)Carvalho, Alex V. [UNESP]Scalvi, Luis V. A. [UNESP]Maciel Jr., Jorge L. B. [UNESP]2022-04-28T20:48:13Z2022-04-28T20:48:13Z2008-01-01info:eu-repo/semantics/publishedVersioninfo:eu-repo/semantics/conferenceObject548-553Materials Science Forum, v. 591-593, p. 548-553.1662-97520255-5476http://hdl.handle.net/11449/2253852-s2.0-58149129022Scopusreponame:Repositório Institucional da UNESPinstname:Universidade Estadual Paulista (UNESP)instacron:UNESPengMaterials Science Foruminfo:eu-repo/semantics/openAccess2024-04-25T17:40:55Zoai:repositorio.unesp.br:11449/225385Repositório InstitucionalPUBhttp://repositorio.unesp.br/oai/requestopendoar:29462024-04-25T17:40:55Repositório Institucional da UNESP - Universidade Estadual Paulista (UNESP)false |
dc.title.none.fl_str_mv |
Powder diffraction of components subject to corrosion in fuse cutouts with ceramiclnsulation |
title |
Powder diffraction of components subject to corrosion in fuse cutouts with ceramiclnsulation |
spellingShingle |
Powder diffraction of components subject to corrosion in fuse cutouts with ceramiclnsulation Carvalho, Alex V. [UNESP] Ceramic Corrosion Fuse cutouts Mullite X-ray diffraction |
title_short |
Powder diffraction of components subject to corrosion in fuse cutouts with ceramiclnsulation |
title_full |
Powder diffraction of components subject to corrosion in fuse cutouts with ceramiclnsulation |
title_fullStr |
Powder diffraction of components subject to corrosion in fuse cutouts with ceramiclnsulation |
title_full_unstemmed |
Powder diffraction of components subject to corrosion in fuse cutouts with ceramiclnsulation |
title_sort |
Powder diffraction of components subject to corrosion in fuse cutouts with ceramiclnsulation |
author |
Carvalho, Alex V. [UNESP] |
author_facet |
Carvalho, Alex V. [UNESP] Scalvi, Luis V. A. [UNESP] Maciel Jr., Jorge L. B. [UNESP] |
author_role |
author |
author2 |
Scalvi, Luis V. A. [UNESP] Maciel Jr., Jorge L. B. [UNESP] |
author2_role |
author author |
dc.contributor.none.fl_str_mv |
Universidade Estadual Paulista (UNESP) |
dc.contributor.author.fl_str_mv |
Carvalho, Alex V. [UNESP] Scalvi, Luis V. A. [UNESP] Maciel Jr., Jorge L. B. [UNESP] |
dc.subject.por.fl_str_mv |
Ceramic Corrosion Fuse cutouts Mullite X-ray diffraction |
topic |
Ceramic Corrosion Fuse cutouts Mullite X-ray diffraction |
description |
Aiming identification of the components most affected by corrosion under saline environment conditions, we have carried out X-ray diffraction measurements in ceramic and bond materials, all in the powder form. The ceramic is analyzed before and after thermal annealing at 1000°C, showing the same DRX peaks, although better defined after annealing. Identification suggests the presence of Al6Si2O13 (Mullite) and SiO 2 (Quartz). Analysis of the junction (bond) material shows similar peaks, but a metallic preponderance is observed. Thermal annealing of the junction is done at much lower temperature, because it melts in the range 135°C-170°C, when a whitish smoke begins to show up along with strong sulfur odor. |
publishDate |
2008 |
dc.date.none.fl_str_mv |
2008-01-01 2022-04-28T20:48:13Z 2022-04-28T20:48:13Z |
dc.type.status.fl_str_mv |
info:eu-repo/semantics/publishedVersion |
dc.type.driver.fl_str_mv |
info:eu-repo/semantics/conferenceObject |
format |
conferenceObject |
status_str |
publishedVersion |
dc.identifier.uri.fl_str_mv |
Materials Science Forum, v. 591-593, p. 548-553. 1662-9752 0255-5476 http://hdl.handle.net/11449/225385 2-s2.0-58149129022 |
identifier_str_mv |
Materials Science Forum, v. 591-593, p. 548-553. 1662-9752 0255-5476 2-s2.0-58149129022 |
url |
http://hdl.handle.net/11449/225385 |
dc.language.iso.fl_str_mv |
eng |
language |
eng |
dc.relation.none.fl_str_mv |
Materials Science Forum |
dc.rights.driver.fl_str_mv |
info:eu-repo/semantics/openAccess |
eu_rights_str_mv |
openAccess |
dc.format.none.fl_str_mv |
548-553 |
dc.source.none.fl_str_mv |
Scopus reponame:Repositório Institucional da UNESP instname:Universidade Estadual Paulista (UNESP) instacron:UNESP |
instname_str |
Universidade Estadual Paulista (UNESP) |
instacron_str |
UNESP |
institution |
UNESP |
reponame_str |
Repositório Institucional da UNESP |
collection |
Repositório Institucional da UNESP |
repository.name.fl_str_mv |
Repositório Institucional da UNESP - Universidade Estadual Paulista (UNESP) |
repository.mail.fl_str_mv |
|
_version_ |
1797790028473040896 |